Bright bar chemical composition by grade
Carbon, silicon, manganese, sulphur, phosphorus, chromium, molybdenum and nickel ranges for the grades we draw, with the standard each one comes from.
This chart gives the chemical composition ranges for 24 bright bar grades as published in BS 970, EN 10083, EN 10084, SAE J403 and J404, IS 2062 and EN 10025. They are the standards' permitted limits. The actual ladle analysis for the heat you receive is stated on the Mill Test Certificate issued with your order.
Composition by grade
All figures are weight per cent. Ranges are those given in the standard named in the last column. Where a dash appears, the element is not specified for that grade.
| Grade | C | Si | Mn | S | P | Cr | Mo | Ni | Other | Standard |
|---|---|---|---|---|---|---|---|---|---|---|
| EN1A | 0.15 max | 0.10 max | 0.90–1.30 | 0.20–0.30 | 0.07 max | – | – | – | – | BS 970 230M07 |
| EN1A Leaded | 0.15 max | 0.10 max | 0.90–1.30 | 0.20–0.30 | 0.07 max | – | – | – | Pb 0.15–0.35 | BS 970 230M07 Pb |
| EN8M | 0.32–0.40 | 0.10–0.35 | 1.00–1.40 | 0.12–0.20 | 0.06 max | – | – | – | – | BS 970 212M36 |
| EN15AM | 0.32–0.40 | 0.10–0.35 | 1.30–1.70 | 0.12–0.20 | 0.06 max | – | – | – | – | BS 970 216M36 |
| SAE 1144 | 0.40–0.48 | – | 1.35–1.65 | 0.24–0.33 | 0.04 max | – | – | – | – | SAE J403 |
| SAE 1018 | 0.15–0.20 | – | 0.60–0.90 | 0.05 max | 0.04 max | – | – | – | – | SAE J403 |
| SAE 1020 | 0.18–0.23 | – | 0.30–0.60 | 0.05 max | 0.04 max | – | – | – | – | SAE J403 |
| SAE 1030 | 0.28–0.34 | – | 0.60–0.90 | 0.05 max | 0.04 max | – | – | – | – | SAE J403 |
| C35 | 0.32–0.39 | 0.40 max | 0.50–0.80 | 0.035 max | 0.035 max | – | – | – | – | EN 10083-2 |
| EN8D / C40 | 0.36–0.44 | 0.40 max | 0.60–1.00 | 0.035 max | 0.035 max | – | – | – | – | BS 970 080M40, EN 10083-2 |
| C45 | 0.42–0.50 | 0.40 max | 0.50–0.80 | 0.035 max | 0.035 max | – | – | – | – | EN 10083-2 |
| SAE 1541 | 0.36–0.44 | – | 1.35–1.65 | 0.05 max | 0.04 max | – | – | – | – | SAE J403 |
| EN9 / C55 | 0.50–0.60 | 0.40 max | 0.50–0.80 | 0.035 max | 0.035 max | – | – | – | – | BS 970 070M55, EN 10083-2 |
| C60 | 0.57–0.65 | 0.40 max | 0.60–0.90 | 0.035 max | 0.035 max | – | – | – | – | EN 10083-2 |
| 16MnCr5 | 0.14–0.19 | 0.40 max | 1.00–1.30 | 0.035 max | 0.025 max | 0.80–1.10 | – | – | – | EN 10084 (1.7131) |
| 20MnCr5 | 0.17–0.22 | 0.40 max | 1.10–1.40 | 0.035 max | 0.025 max | 1.00–1.30 | – | – | – | EN 10084 (1.7147) |
| 40Cr4 / EN18 | 0.35–0.45 | 0.40 max | 0.60–0.90 | 0.035 max | 0.035 max | 0.90–1.20 | – | – | – | BS 970 530M40, EN 10083-3 |
| EN19 | 0.36–0.44 | 0.10–0.35 | 0.70–1.00 | 0.04 max | 0.035 max | 0.90–1.20 | 0.25–0.35 | – | – | BS 970 709M40 |
| 42CrMo4 | 0.38–0.45 | 0.40 max | 0.60–0.90 | 0.035 max | 0.025 max | 0.90–1.20 | 0.15–0.30 | – | – | EN 10083-3 (1.7225) |
| EN24 | 0.36–0.44 | 0.10–0.35 | 0.45–0.70 | 0.04 max | 0.035 max | 1.00–1.40 | 0.20–0.35 | 1.30–1.70 | – | BS 970 817M40 |
| EN31 | 0.90–1.20 | 0.10–0.35 | 0.30–0.75 | 0.04 max | 0.035 max | 1.00–1.60 | – | – | – | BS 970 534A99 |
| SAE 52100 | 0.93–1.05 | 0.15–0.35 | 0.25–0.45 | 0.025 max | 0.025 max | 1.35–1.60 | – | – | – | SAE J404 |
| IS 2062 E250 | 0.23 max | 0.40 max | 1.50 max | 0.045 max | 0.045 max | – | – | – | – | IS 2062 |
| ST 52.3 / S355J2 | 0.20 max | 0.55 max | 1.60 max | 0.025 max | 0.025 max | – | – | – | – | EN 10025-2 |
How to read this table. These are the ranges given in the published standards, reproduced here as a buyer reference. They are not Akansha Ispat certified values. The actual chemistry and properties of the steel you receive are stated on the Mill Test Certificate issued with your order, and standards are revised from time to time, so a controlled copy of the current standard governs in any dispute.
Reading a composition like a metallurgist
Carbon (C)
The single most important number. It sets how hard the steel can get. Below about 0.25 per cent the steel will not through harden and is carburised instead. From 0.35 to 0.55 per cent it responds to quenching and tempering. Around 1.0 per cent, as in EN31, it gives bearing hardness.
Manganese (Mn)
Raises hardenability, so a thicker section hardens through to the centre. It also combines with sulphur to form the inclusions free cutting steels rely on. High manganese grades such as SAE 1541 are chosen for strength without alloy cost.
Sulphur (S)
An impurity in most grades, capped at 0.035 per cent, and a deliberate addition in free cutting grades at 0.20 to 0.33 per cent. It improves machinability and reduces transverse ductility. Which of those matters depends entirely on the part.
Chromium (Cr)
Increases hardenability and wear resistance, and forms hard carbides. It is what separates EN19 and EN24 from plain carbon steels, and at 1.0 to 1.6 per cent in EN31 it gives the carbide structure a bearing race needs.
Molybdenum (Mo)
Added at 0.15 to 0.35 per cent to resist temper embrittlement and to hold strength at elevated temperature. It is the reason EN19 and 42CrMo4 are specified for highly stressed shafts rather than a plain chromium steel.
Phosphorus (P)
Generally an unwanted residual, capped at 0.035 per cent or lower, because it embrittles grain boundaries. The exception is free cutting steels, where a slightly higher limit is tolerated for machinability.
Composition is a means, not an end
Most buyers do not actually want a composition, they want a part that lasts. The quickest route is usually to start from the duty and work back.
- High volume turned parts, light duty. Free cutting: EN1A, EN1A leaded, EN8M.
- General shafts and spindles. Medium carbon: EN8D, C45.
- Gears and parts needing a hard skin on a tough core. Case hardening: 16MnCr5, 20MnCr5.
- Highly stressed shafts and couplings. Alloy: EN19, 42CrMo4, EN24.
- Bearing races and rollers. Bearing: EN31, SAE 52100.
- Fabricated and structural parts. Mild: IS 2062, ST 52.3, SAE 1018.
Related reference
- Grade equivalence chart, if your drawing uses SAE, DIN or JIS designations
- Tolerance classes h6 to h12
- IS 9550, the bright bar product standard
- EN8 vs EN8D vs EN19 explained
Common questions
What is the chemical composition of EN8D?
EN8D is a medium carbon steel with typically 0.36 to 0.44 per cent carbon, 0.60 to 1.00 per cent manganese, up to 0.40 per cent silicon, and sulphur and phosphorus each limited to 0.035 per cent. It corresponds to 080M40 in BS 970 and C40 in EN 10083-2.
What is the difference between EN8 and EN8D in composition?
They sit in the same carbon range. EN8D is the more closely controlled variant, supplied to tighter limits on carbon and on residual elements, which makes its response to heat treatment more consistent from heat to heat.
Why does EN1A have so much sulphur?
Deliberately. The sulphur forms manganese sulphide inclusions that break the chip as it forms, which is what makes EN1A a free cutting steel. The same inclusions reduce transverse ductility, so EN1A is not used where the part is loaded across the bar axis.
Does the Mill Test Certificate give the actual composition?
Yes. The MTC states the ladle analysis for the specific heat your bars came from, which is the authoritative figure for that material. The ranges on this page are the standard's permitted limits, not the values of any particular heat.
Which grades are case hardening grades?
16MnCr5 and 20MnCr5 are the case hardening grades in this range. Their carbon is low, around 0.14 to 0.22 per cent, so the core stays tough while carburising builds a hard surface layer.
Tell us the grade, size and quantity.
Send your requirement and our team will reply with availability and a quotation. Share a drawing if you have one.
+91 98193 91906