Every bright bar starts life as a hot rolled black bar. To make it bright, the mill either cold draws it through a die or peels off its outer layer. Both give a clean, accurate bar, but they change the material in different ways. Picking the right one saves machining time and avoids rejections later.
What is a cold drawn bar?
A cold drawn bar is descaled and then pulled through a hardened die at room temperature. The die squeezes the bar down to a slightly smaller, very accurate size and shape.
- Tight size control. Drawing gives consistent diameters and sharp, accurate square and hex sections.
- Higher surface strength. Cold working raises tensile and yield strength near the surface.
- Smooth finish. The die leaves a bright, polished surface.
- Any profile. Round, square and hexagonal bars can all be drawn.
The trade-off: drawing does not remove material, so any seams or decarburisation on the hot rolled surface stay in the bar. Drawing also leaves some residual stress, which can show up as slight movement when you machine one side of a part heavily.
What is a peeled bar?
A peeled bar has its outer skin turned off on a peeling machine, then is straightened and polished. Peeling removes mill scale, surface seams and the decarburised layer, so the material is sound right to the surface.
- Defect free surface. Ideal for parts that will be induction hardened, plated or highly stressed.
- No cold work. Mechanical properties stay close to the hot rolled or heat treated condition.
- Larger sizes. Peeling is common for bigger diameters where drawing is less practical.
- Round only. Peeling works on round bars, not square or hex.
Side by side
| Factor | Cold drawn | Peeled |
|---|---|---|
| Profiles | Round, square, hex | Round only |
| Size accuracy | Very good | Very good |
| Surface defects and decarb | Remain from hot rolled bar | Removed |
| Strength | Increased by cold work | Unchanged from hot rolled or heat treated state |
| Residual stress | Some | Low |
| Best for | Turned parts, pins, keys, fasteners, fittings | Large or critical shafts, induction hardened and plated parts |
How to choose
- Need square or hex? Choose cold drawn.
- Will the part be induction hardened, chrome plated or fatigue loaded? Choose peeled, so no surface defect is hardened in.
- Small to medium round parts machined in high volume? Cold drawn gives size, finish and strength at a good cost.
- Large diameters? Peeled is usually the practical choice.
Still unsure? Send us your drawing. Akansha Ispat makes both cold drawn and peeled bright bars and can suggest the right route for your part.
Frequently asked questions
Is a peeled bar better than a cold drawn bar?
Neither is better in every case. Peeled bars have a defect free surface and suit critical, hardened or plated parts. Cold drawn bars have higher surface strength, come in more profiles and suit most turned parts.
Can square and hex bars be peeled?
No. Peeling works only on round bars. Square and hexagonal bright bars are cold drawn.
Does cold drawing increase strength?
Yes. Cold drawing work hardens the bar, raising tensile and yield strength, especially near the surface.